Non-polar a-plane GaN Grown by HVPE on r-plane Sapphire Substrates: Substrate Selection, Pre-treatment, and Epitaxial Challenges

published on 2026-11-26

1. Why Non-polar a-plane GaN Is Needed

In conventional c-plane GaN devices, spontaneous and piezoelectric polarization act along the crystallographic orientation, giving rise to the quantum-confined Stark effect (QCSE). Within the quantum wells, the electron and hole wavefunctions are strongly separated in space, which ultimately lowers the internal quantum efficiency of the device. Using a non-polar GaN epilayer can weaken—or even eliminate—this polarization field at its source, making non-polar GaN a highly promising material route for green LEDs and high-stability optoelectronic devices.
 

Figure 1. Comparison of polarization-field-induced electron–hole wavefunction separation in c-plane GaN with the negligible polarization field in non-polar a-plane GaN.
 

2. Why r-plane (1−102) Sapphire Was Chosen as the Foreign Substrate

There are two principal routes to non-polar GaN substrates. The first is slicing bulk polar GaN along non-polar orientations; however, this route suffers from low throughput and limited wafer size, which makes commercialization difficult. The second is heteroepitaxy of non-polar GaN on foreign substrates, which can be implemented by MOCVD, MBE, or HVPE. Among these, HVPE offers a high growth rate and high throughput and is regarded as one of the most industrially promising routes.
Among foreign substrates, r-plane (1−102) sapphire provides crystallographic matching with a-plane (11−20) GaN and offers the following practical advantages:
  • Low cost, availability of large-size wafers, and compatibility with existing production-line equipment;
  • When combined with high-rate HVPE growth, it holds promise for large-scale, low-cost supply of a-plane GaN templates;
  • Thick non-polar GaN templates are in clear demand for high-throughput epitaxial processes.
This hetero-system nevertheless has intrinsic drawbacks. The large difference in lattice mismatch between the two orthogonal in-plane directions produces anisotropic strain, which readily triggers extended defects such as stacking faults and threading dislocations; the defect level in early samples directly constrained device performance.


3. Substrate Pre-treatment and Epitaxial Process

In this experiment, 2-inch r-plane (1−102) sapphire substrates were processed in a vertical down-flow HVPE reactor with a 6-inch chamber diameter. To relieve the significant stress arising during heteroepitaxy of non-polar GaN, the substrates received an in-situ surface pre-treatment before growth:
  1. HCl gas etching at a flow rate of 70 sccm;
  1. NH₃ nitridation at a flow rate of 2500 sccm for 5 min.
This pre-treatment forms a discontinuous GaN nano-dot buffer layer on the sapphire surface. SEM characterization confirms that discrete nano-dots first form on the substrate; subsequent GaN nucleates on these dots and coalesces laterally, ultimately yielding a 5-μm-thick a-plane GaN epilayer. The main growth conditions are summarized below.
Process parameter Value
Growth temperature ~1080 °C
Growth pressure Atmospheric pressure
V/III ratio ~6
HCl flow rate (GaCl generation) 40 sccm (GaCl conversion efficiency ~15%)
Total N₂ carrier-gas flow 15000 sccm
Epilayer thickness 5 μm
Stacking fault density 4.12 × 10⁵ cm⁻¹
Threading dislocation density 3.86 × 10⁹ cm⁻²
 
 
The resulting stacking-fault and dislocation levels are on the same order of magnitude as those of a-plane GaN grown by MOCVD. This shows that the pre-growth strategy—HCl etching plus nitridation to construct a GaN nano-dot buffer layer—can deliver acceptable crystal quality on r-plane sapphire.

 

Figure 2. Cross-sectional schematic of the substrate–buffer–epilayer stack: from top to bottom, the 5-μm a-plane GaN epilayer, the discontinuous GaN nano-dot buffer layer, and the 2-inch r-plane (1−102) sapphire substrate.
 

4. The Central Trade-off of the Sapphire System: High Throughput vs. Defect Risk

Advantages: r-plane sapphire is inexpensive and available in large sizes; together with high-rate HVPE growth, it offers a realistic pathway to low-cost mass production of non-polar a-plane GaN templates.
Risk factors:
  • Anisotropic lattice mismatch directly induces extended defects such as stacking faults and dislocations;
  • Quartz tubing inside the HVPE reactor introduces unintended oxygen impurities, while carbon and silicon impurities may also enter through the substrate and reactor ambience;
  • High-rate growth favors the formation of intrinsic point defects such as gallium vacancies () and nitrogen antisites (). These defects act as deep traps that capture carriers and degrade the performance of LEDs and power devices.
A long-standing view in the industry holds that a-plane GaN produced by high-rate HVPE inevitably exhibits markedly inferior electrical and optical performance to its MOCVD-grown counterpart. The core value of this paper lies in a quantitative deep-level transient spectroscopy (DLTS) assessment of whether, on the r-plane sapphire system, HVPE can suppress deep-trap levels down to the MOCVD benchmark.


5. Summary

r-plane sapphire is not an ideal substrate, but it is an indispensable cornerstone on the path to practical non-polar GaN. HCl etching followed by nitridation to form a GaN nano-dot buffer layer is the critical pre-processing step that determines the success of this HVPE process. Even after extended defects are partially suppressed, heteroepitaxy still introduces intrinsic point defects; the type and concentration of these traps directly set the performance ceiling of the resulting devices.
 
1


R-plane Sapphire Substrates and Related Supply

The r-plane (1−102) sapphire substrates discussed in this article fall within the standard supply range of  JXT, JXT is a technology-oriented enterprise focused on semiconductor wafer processing and epitaxial technology. It has long supplied 2–12-inch sapphire substrates covering c-plane (0001), r-plane (1−102), m-plane (1−100), and a-plane (11−20) orientations, with customization of special orientations and off-cut angles available to meet the orientation and miscut precision requirements of non-polar/semi-polar GaN epitaxy.
In terms of surface quality, JXT delivers wafers through the full process chain of multi-wire slicing → lapping → CMP polishing. The CMP-polished wafers typically exhibit a surface roughness Ra better than 0.5 nm, with high-end products reaching below 0.2 nm; they show an atomically stepped surface morphology free of scratches and plastic-damage layers, ready for direct GaN epitaxy. The company also provides sapphire laser dicing and customization of dimensions and crystal orientations.
Beyond sapphire substrates, its product portfolio covers SiC monocrystalline substrates, diamond substrates and films, quartz and fused silica, SOI, lithium tantalate/lithium niobate, as well as bonding services (e.g., Si-on-SiC), enabling material combinations tailored to different device routes.
 
Product Specification range Remarks
Sapphire monocrystal substrates (standard / special orientations) 2–12 inch; c (0001), r (1−102), m (1−100), a (11−20) The 2-inch r-plane substrate used here is a standard product; the orientation can be selected for the specific epitaxy system.
Off-cut substrates 2–6 inch; off-cut 0.5°–6°, tolerance ±0.1° For heteroepitaxy and special device structures sensitive to miscut angles.
Patterned sapphire substrates (PSS / NPSS) 2–4 inch; c-plane miscut 0.2° ± 0.1° toward the m-axis Patterned solution for enhancing LED light-extraction efficiency.
Sapphire wafer carriers / optical windows Carriers 3–12 inch; windows 50.8–152 mm, etc. For epitaxy fixtures, metrology carriers, and optical-window applications.
 
 
 
 